Time to Delamination (T260 / T288)
Quality & Inspection Standards
PRODUCTS CENTER
Get Custom Quote
PRODUCTS CENTER
Time to Delamination (T260 / T288) – TMA Method & IPC Acceptance
Time to delamination (T260 and T288) is one of the most under‑specified but critical material properties for high‑reliability PCBs. It measures how many minutes a laminate can withstand 260°C or 288°C before internal layers separate. We have seen aerospace programs reject entire material lots because T260 dropped from >60 minutes to <15 minutes after improper storage. Per IPC‑4101, minimum T260 is 30 minutes for many high‑Tg materials. This guide explains the TMA test method (IPC‑TM‑650 2.4.24.1), typical values for different resin systems, and how to use T260/T288 in material selection.
Table of Contents
1. What Are T260 and T288? – Definition and Physics
T260 and T288 are time‑to‑delamination values measured by thermomechanical analysis (TMA). A small laminate sample (≈6.35mm square) is heated rapidly to 260°C or 288°C and held at that temperature while a probe monitors thickness expansion. When delamination occurs, the thickness suddenly increases (or the probe penetrates). The time from reaching the set temperature to the onset of delamination is recorded.
- T260: Resistance to delamination at 260°C – typical lead‑free reflow peak.
- T288: More severe, used for high‑temperature applications (e.g., multiple reflows, aerospace).
A longer T260/T288 means the laminate can survive longer at peak reflow temperature without internal separation. Per IPC‑4101, many FR‑4 materials have T260 ≥30 minutes. High‑reliability materials (polyimide, high‑Tg epoxy) often exceed 60 minutes. Materials with poor T260 (<5 minutes) will likely delaminate during assembly.
2. TMA Test Method (IPC‑TM‑650 2.4.24.1)
IPC‑TM‑650 2.4.24.1 specifies the TMA procedure:
- Sample: ≈6.35mm × 6.35mm, thickness ≥0.5mm (preferably 1.6mm). For thin laminates, stack layers.
- Pre‑bake: 105°C for 2 hours to remove moisture.
- Ramp rate: 10°C/min from 35°C to the set temperature (260°C or 288°C).
- Dwell: Hold at set temperature until delamination occurs or 60 minutes (or specified limit).
- Delamination detection: A sudden expansion >0.025mm or a change in slope of the expansion curve.
Figure 1 in the method shows a typical TMA curve: thickness remains stable, then abruptly increases at delamination. The time at temperature is recorded as T260 or T288.
Typical TMA curve for epoxy laminate at 260°C:
Thickness → stable → sudden jump → delamination
In our lab, we have seen that samples with poor lamination pressure show T260 under 10 minutes, while properly processed samples exceed 45 minutes. The test is sensitive to sample preparation – rough edges cause early failure.
3. Typical T260/T288 Values by Material
Values vary widely by resin system and cure. The table below shows typical ranges from industry data (not IPC‑mandated).
| Material Type | T260 (min) | T288 (min) | Typical Application |
|---|---|---|---|
| Standard FR‑4 (Tg 130‑140°C) | 10‑25 | <5 | Consumer, single reflow |
| Mid‑Tg FR‑4 (150‑170°C) | 20‑40 | 5‑15 | Industrial, telecom |
| High‑Tg FR‑4 (170‑180°C) | 30‑60+ | 10‑30 | Server, automotive |
| Lead‑free compatible (180°C+) | 60+ | 30‑60 | High‑reliability, multiple reflow |
| Polyimide / BT / Cyanate ester | 90+ | 60+ | Aerospace, military |
Table 1: Typical T260/T288 values. Verify with your material supplier's datasheet – not all materials are tested to these temperatures.
Engineering Insight
A high T260 does not guarantee good T288. We have seen FR‑4 materials with T260 >45 minutes but T288 <5 minutes. If your assembly requires multiple 260°C reflows, specify both T260 and T288.
4. What Reduces T260/T288 – Moisture, Cure, Contamination
Through our incoming material qualification, we have identified three primary factors that degrade time to delamination:
- Moisture absorption: Prepreg stored >6 months in humid conditions (>50% RH) can absorb >0.5% moisture. During TMA, water vaporizes and forces delamination. Per IPC‑4101, moisture content should be <0.2% for most materials. We have seen T260 drop from 45 minutes to 12 minutes after 3 months of uncontrolled storage.
- Incomplete cure (under‑cured laminate): Low lamination temperature or short press time leaves unreacted resin that decomposes at 260°C, generating gas and causing delamination. DSC per IPC‑TM‑650 2.4.25 can verify cure. A ΔTg >5°C indicates under‑cure.
- Contamination (oil, grease): Innerlayer contamination prevents proper bonding. Microsection after TMA will show separation at the contaminated interface.
In one program, a supplier substituted a lower‑grade prepreg without notifying us. The T260 dropped from 52 minutes (certified) to 18 minutes. We caught it during incoming inspection and rejected the entire lot – saving a potential field failure.
5. Acceptance Criteria: IPC‑4101 and Customer Specs
IPC‑4101 (the laminate specification) defines minimum T260 and T288 for each material type (e.g., for FR‑4 types). However, many customers impose stricter limits. Common requirements:
| Product Class | Minimum T260 (min) | Minimum T288 (min) | IPC Reference |
|---|---|---|---|
| Class 2 (standard) | 15 or per datasheet | Not specified | AABUS |
| Class 3 (high reliability) | ≥30 | ≥10 | Common OEM requirement |
| Aerospace / IPC‑6012ES | ≥60 | ≥30 | AS9100 / customer |
| Automotive under‑hood | ≥30 (at 260°C) | ≥15 | AEC‑Q100 derived |
Table 2: Typical minimum T260/T288 by application. Always specify in your procurement document.
Note: IPC‑6012E does not directly mandate T260/T288 testing for production boards – it is a material qualification test per IPC‑4101. However, many OEMs require laminate T260/T288 data as part of the incoming inspection.
T260/T288 Qualification Checklist (IPC‑Anchored)
- Request T260 and T288 data from laminate supplier. Do not assume "high Tg" means good T288.
- Specify minimum values in your material callout. Example: "Laminate per IPC‑4101/126, T260 ≥30 min, T288 ≥10 min."
- Verify test method. Ensure supplier uses IPC‑TM‑650 2.4.24.1, not an internal method.
- Perform incoming TMA on first article. We have caught counterfeit materials with low T260.
- Monitor prepreg storage conditions. Moisture reduces T260 significantly. Use dry cabinets.
- If T260 fails, run DSC to check cure. Under‑cured material often shows low T260.
- Document TMA curves. Include in qualification report.
6. FAQ
Q: What is the difference between T260 and Tg?
A: Tg (glass transition temperature) is the temperature where the resin changes from rigid to rubbery. T260 measures how long the laminate can survive at 260°C before delamination. A high Tg (>170°C) is necessary but not sufficient for good T260 – cure and moisture also matter.
Q: Can I use T260 to predict field life?
A: Indirectly. Low T260 (<10 min) indicates the material will likely delaminate during assembly reflow. For field life (thermal cycling), T260 alone is not sufficient – you need thermal shock testing per IPC‑TM‑650 2.6.7.2. However, materials with very low T260 often also fail thermal cycling early.
Q: Is T288 required for all PCBs?
A: No. T288 is typically required for high‑temperature applications (e.g., multiple lead‑free reflows, automotive under‑hood, aerospace). For single‑reflow consumer products, T260 is sufficient.
Q: What is the typical T260 for standard FR‑4?
A: Most standard FR‑4 (Tg 130‑140°C) has T260 between 10 and 25 minutes. However, many low‑cost laminates do not specify T260 – they may delaminate in seconds. Always ask for data.
Continue Reading – Thermal Reliability Series
Related Manufacturing Capability
Controlled laminate selection, prepreg construction, lamination process and thermal-reliability management for complex multilayer PCB builds.
If T260, T288, Tg, Td or repeated lead-free reflow exposure is a reliability concern, submit the laminate system and production stackup for an engineering review before fabrication.
Request Thermal Reliability Review →References: IPC‑TM‑650 2.4.24.1; IPC‑4101 (laminate specification); IPC‑6012E §3.2.3; IPC‑6018 §5.2. IPC‑TM‑650 Official Method.